Just click the link(s) for pictures...

The 32Rem... http://castboolits.gunloads.com/atta...5&d=1395962456

225Win.... http://castboolits.gunloads.com/atta...6&d=1435950318

Both are made from the 30-30 parent case. What I do is knock the shoulder longer through Hydroforming.

The 225 shoulder is .090 longer than the 30-30 so I make what I need and fill the case with water, run it up in the die, insert the plunger, whack it with my brass hammer, and the shear force forces it to shape. The only other way to form them is to fire form them, and I don't own anything in most of the conversions I do....